Export Control
EAR Export Classification: Not subject to the EAR per 15 C.F.R. Chapter 1, Part 734.3(b)(3), except for the following Service Bulletins which are currently published as EAR Export Classification 9E991: SBE70-0992, SBE72-0483, SBE72-0580, SBE72-0588, SBE72-0640, SBE73-0209, SBE80-0024 and SBE80-0025.Copyright
© IAE International Aero Engines AG (2001, 2014 - 2021) The information contained in this document is the property of © IAE International Aero Engines AG and may not be copied or used for any purpose other than that for which it is supplied without the express written authority of © IAE International Aero Engines AG. (This does not preclude use by engine and aircraft operators for normal instructional, maintenance or overhaul purposes.).Applicability
All
Common Information
TASK 72-50-22-300-145 LPT Stage 4 Vane - Touch-Up Coat Repair, Repair-145 (VRS4615)
General
Price and availability - none
The practices and processes referred to in the procedure by the TASK numbers are in the SPM.
Make sure that the necessary cleaning and inspection procedures are done before this repair.
NOTE
Preliminary Requirements
Pre-Conditions
NONESupport Equipment
NONEConsumables, Materials and Expendables
NONESpares
NONESafety Requirements
NONEProcedure
Refer to SPM TASK 70-38-14-380-501.
Prepare the material and the surface.
SUBTASK 72-50-22-330-004 Prepare the Material and Surfaces
Refer to Figure.
Refer to SPM TASK 70-38-14-380-501.
Apply coating in area A1.
SUBTASK 72-50-22-380-004 Touch-Up Coating of the Stage 4 Turbine Vane
Refer to SPM TASK 70-38-14-380-501.
Diffuse the recoated stage 4 turbine vane
Refer to SPM TASK 70-37-27-370-501, except temperature range to be 1625 deg F to 1675 deg F (885 deg C to 913 deg C) for eight hours.
Precipitation heat treat the stage 4 turbine vane.
SUBTASK 72-50-22-370-006-001 Diffusion Heat Treatment of the Recoated Stage 4 Turbine Vane
NOTE
Before diffusion heat treatment remove the honeycomb, refer to Repair VRS4577 TASK 72-50-22-300-126 (REPAIR-126).After diffusion heat treatment replace the honeycomb, refer to Repair VRS4577 TASK 72-50-22-300-126 (REPAIR-126).NOTE
Do the precipitation heat treatment after all braze operations.Refer to SPM TASK 70-38-14-380-501 except diffusion heat treat at 1575 deg F to 1625 deg F (857 deg C to 885 deg C) for two hours.
Diffuse the recoated stage 4 turbine vane.
SUBTASK 72-50-22-370-006-002 Diffusion Heat Treatment of the Recoated Stage 4 Turbine Vane
NOTE
Precipitation heat treatment is not necessary.Refer to SPM TASK 70-38-14-380-501.
Examine the recoated areas.